Introduction
Laser powder bed fusion (LPBF) technology is one of the most fastest growing technologies in metal additive manufacturing, which can produce critical stainless steel components for reactor in-cores with complex shapes, helping to achieve integrated manufacturing and rapid prototyping, providing new options and opportunities to overcome the bottleneck of traditional processing technology. Therefore, it has attracted widespread attention in the field of nuclear power plants [1, 2]. Austenitic stainless steel is used as the key structural material for reactor core components owing to its excellent high-temperature mechanical and corrosion resistance properties [3]. Furthermore, the service environment involves high-flux and long-term neutron irradiation and is susceptible to (n, a) transmutation reactions with the material, which inevitably produce an abundance of helium atoms in the structural material. Helium is an inert element that does not combine with other atoms or dissolve in the material matrix. As the concentration of helium atoms continues to accumulate and precipitate, helium vacancy clusters are formed and ultimately agglomerate into helium bubbles [4, 5]. Helium bubbles are prone to aggregation and coarsening at grain boundaries, phase boundaries, and dislocations, which seriously alters the microstructure of the material and leads to surface foaming [6], expansion [7, 8] and helium embrittlement [9, 10], reducing the mechanical properties of the material and seriously affecting the safety and economy of nuclear power plants.
It is widely known that nanoscale ultrafine structure possesses high-volume fraction interfaces, including grain boundaries, phase boundaries, and layer interfaces, which can serve as defect sinks to improve radiation resistance [11]. Zinkle et al. [12] also demonstrated that nanocrystalline materials, oxide dispersion strengthened (ODS) steel, and nanostructured ferrite alloys exhibit high defect sinking strength
Therefore, it is necessary to elucidate the dependence of helium bubbles on annealing time and the evolution of the microstructure of LPBF-processed stainless steels. In this study, 350 keV He+ ions were injected into LPBF 304L stainless steel and conventionally rolled 304 L stainless steel samples at a flux of 1×1017 ions/cm2 at room temperature and annealed at 750 °C for 10, 100, and 300 h, respectively. The coarsening behavior of the helium bubbles in the LPBF and rolled samples was compared. Cross section TEM (transmission electron microscopy) analysis showed that the LPBF sample exhibited superior resistance to helium bubble growth.
Experiment
Sample preparation
The 304L stainless steel LPBF samples in this study were manufactured using an EOS M280 machine in an argon gas atmosphere. Gas-atomized powder with a particle size ranging from 10 to 53 μm was utilized as the feedstock powder, and the printing parameters and chemical composition have been described in previous publications [20]. The LPBF and rolled sample (cut from a commercial 304L plate rolled at room temperature) were sectioned into small sample dimensions of 2 mm×5 mm×1 mm using wire-cutting techniques. The sample was gradually ground with 220–3000 grit sandpaper and polished with
Helium ion implantation and annealing
The surfaces of the samples were mirror-polished, irradiated with raster beams, and then implanted with 350 keV helium ions at room temperature with a fluence of 1 × 1017 ions/cm2 at the Institute of Semiconductors, Chinese Academy of Science. Details of the implantation test are provided in a previous publication [33]. Helium ion irradiation damage and He concentration profiles were calculated using SRIM (the Stopping and Range of Ions in Matter) [34] and are shown in Fig. 1. The peak ion concentration was approximately 0.8–0.9 μm away from the sample surface. The highest concentration of He was approximately 5.6 at%, and the maximum damage depth was approximately 1 μm beneath the surface. The samples were then annealed for 10, 100, and 300 h in a tube furnace at 700°C to gain insight into the helium bubble growth behavior, which were called as PIAed samples. The LPBF and rolled samples for TEM observation were prepared using a focused ion beam (FIB, FEI Nanolab 600) system to characterize the helium bubble density and distribution in the two states of as-irradiation and PIA. To ensure the accuracy of the experimental data, each sample was taken from the same sample within the peak damage zone, and the size and quantity of helium bubbles were measured using image software through several TEM images. The thickness of the TEM samples was determined using convergent beam electron diffraction (CBED). The samples were labeled as T1(Rolled, implanted), T2(Rolled, implanted + PIA at 700 °Cfor 10 h), T3(Rolled, implanted+PIA at 700°C for 100 h), T4 (Rolled, implanted+PIA at 700 °C for 300 h); A1 (LPBF, implanted), A2(LPBF, implanted+PIA at 700 °C for 10 h), A3(LPBF, implanted+PIA at 700 °C for 100 h), A4 (LPBF, implanted+PIA at 700 °C for 300 h). TEM lamella thinness and experimental conditions are listed in Table 1.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F001.jpg)
| Label | Sample Status | Sample thickness (nm) |
|---|---|---|
| T1 | Rolled, implanted | 52 |
| T2 | Rolled, implanted, PIA at 700 °C for 10 h | 50 |
| T3 | Rolled, implanted, PIA at 700 °C for 100 h | 50 |
| T4 | Rolled, implanted, PIA at 700 °C for 300 h | 65 |
| A1 | LPBF, implanted | 52 |
| A2 | LPBF, implanted, PIA at 700 °C for 10 h | 50 |
| A3 | LPBF, implanted, PIA at 700 °C for 100 h | 50 |
| A4 | LPBF, implanted, PIA at 700 °C for 300 h | 65 |
Results
The stability of the microstructure in Laser Powder Bed Fusion samples
LPBF 304L stainless steel generally exhibits finer grain sizes owing to the rapid solidification rates during the LPBF process. The grain size of LPBF 304L stainless steel can range from approximately 1 to 10 μm [35], depending on the laser parameters and scan strategy used [36]. The grain size of stainless steel prepared using traditional processes typically ranges from 10 to 30 μm after recrystallization and annealing processes [37]. In the LPBF process, cellular structures are more easily formed at a relatively high ratio of temperature gradient (G) to cooling rate (R). As shown in Fig. 2, a small amount of nano-oxide particles, cellular subgrains, and linear dislocations were observed in the LPBF 304L stainless steel. In our previous study, we demonstrated that the cellular subgrains are composed of high-density dislocation walls [20]. As shown in Fig. 3, the cellular subgrains in the post-irradiation LPBF sample remained unaltered, indicating that irradiation had no significant influence on the cellular subgrain structure. This is consistent with the research findings of C. Fu. [19].
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F002.jpg)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F003.jpg)
In Fig. 4, the cellular subgrains of LPBF sample are still remained with the size range of approximately 0.5 μm even after annealing for 10 and 100 h, indicating that their structure remain relatively stable even after high-temperature annealing for 100 h. After annealing for 300 h, the cellular subgrains were decomposed, but many dislocations were still present.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F004.jpg)
Helium bubbles in the matrix
Figure 5 shows the distribution of helium bubbles in the two materials after He injection at room temperature. In the T1 rolled samples, the depth of the helium-causing damage zone was approximately 980 nm, and the width was approximately 470 nm. The helium bubble size and density were 1.12 nm in diameter and 3.86×1024 m-3, respectively. In the A1 LPBF samples, the depth of the helium bubble damage zone was approximately 950 nm, the width was approximately 430 nm, and the corresponding data were 1.0 nm in diameter and 1.12 × 1024 m-3 number density, respectively. This result demonstrates that the helium bubble nucleation and damage zone width in the LPBF sample are lower than those in rolled sample, which is consistent with our previous conclusion that the PLBF 304L stainless steel exhibits better irradiation resistance [20]. However, the helium bubble number density of both samples is one order of magnitude higher than that in the literature [20], caused by our higher helium injection dose.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F005.jpg)
As shown in Fig. 6, high magnification TEM images of all samples are taken near a depth range of 700 to 1000 nm for investigating the evolution of helium bubbles, which can be used to quantify the size and density of bubbles and evaluate the effect of annealing time on the behavior of helium bubbles. The specific statistical results are presented in Table 2 and Fig. 7, the TEM results reveal that as the annealing time prolonged, the size of bubbles increase and the density of bubbles decrease.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F006.jpg)
| Label | Sample status | Average size of helium bubbles (nm) | Helium bubble density (m-3) |
|---|---|---|---|
| T1 | Rolled, implanted | 1.12 | 3.86 × 1024 |
| T2 | Rolled, implanted, PIA at 700 °C for 10 h | 1.67 | 1.84 × 1024 |
| T3 | Rolled, implanted, PIA at 700 °C for 100 h | 11.18 | 1.03 × 1023 |
| T4 | Rolled, implanted, PIA at 700 °C for 300 h | 11.6 | 9.12 × 1022 |
| A1 | LPBF, implanted | 1.00 | 1.12 × 1024 |
| A2 | LPBF, implanted, PIA at 700 °C for 10 h | 2.12 | 1.22 × 1023 |
| A3 | LPBF, implanted, PIA at 700 °C for 100 h | 8.5 | 7.76 × 1022 |
| A4 | LPBF, implanted, PIA at 700 °C for 300 h | 8.93 | 6.73 × 1022 |
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F007.jpg)
After annealed at 700 °C to 10 hours, the helium bubble sizes increase from 1.12 nm to 1.67 nm and from 1 nm to 2.12 nm in the rolled and LPBF sample. It is evident that the helium bubbles remain relatively stable after a short soaking time of 10 h in both samples. The size of the helium bubbles in the LPBF sample was slightly larger than that of the rolled sample, but continued to grow in a stable range of helium bubble sizes [38], which had a minimal impact on helium embrittlement. A declining density of helium bubbles occurred in the two states of the samples. The helium bubble density in the LPBF sample was one order of magnitude lower than that in the rolled samples.
After annealing for 100 h, the helium bubble size in the rolled sample increases from 1.67 nm to 11.18 nm while in the LPBF sample from 2.12 nm to 8.5 nm. Significant coarsening of helium bubbles indicated a fast growth of helium bubbles in the 10–100 h annealing stage. The average size of helium bubbles in the two materials (rolled and LPBF samples) with the lowest and highest dislocation structure densitied [20] was coarsened by 6.69 and 4.01 times, respectively. The density decreases from 1.84×1024 m-3 to 1.03 × 1023 m-3 in rolled sample and from 1.22 × 1023 m-3 to 7.76 × 1022 m-3 in LPBF sample with the decrease rate calculated as 94.4%, and 36.4%. Considering the bubble size and density evolution with annealing time, the helium bubbles in the LPBF samples grew steadily after the PIA treatment.
After 300 h of annealing, as shown in Fig. 7, the size and density of the helium bubbles have essentially reached a stable state for both samples, showing no significant alterations. Throughout the annealing process, the helium bubble density and the sensitivity of helium bubble coarsening to annealing time in the LPBF samples were lower than those of the rolled samples, indicating the excellent resistance of the LPBF samples to helium bubble growth.
Helium bubbles on nanoparticles
It is well known that the microstructure affects the behavior of helium bubbles in materials. To elucidate the diversity of the helium bubbles coarsening with increasing annealing time between LPBF and rolled 304L stainless steel, more detailed statistics of helium bubbles combined with the intrinsic structures are needed to assess the influence of the matrix microstructure. The Fig. 8 presents the evolution of the helium bubble nearby the nano-oxide particles in the LPBF samples. It can be observed that there is no significant accumulation of helium bubbles at the oxide-matrix interface without annealing. But a small number of helium bubbles are found to aggregate at the nano-oxide particles after annealing at 700 °C for 10 to 100 hours, as indicated by the white arrows in Fig. 8(b) and (c). However, almost no accumulation of helium bubbles was observed at the oxide-matrix interface through the entire field of view after 300 h. PIAed sample in Fig. 8(d-e-f).
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F008.jpg)
The results indicate that the nano-oxide-matrix interface is a defective sink for trapping helium atoms. The nanoparticles still possess sufficient trapping ability for helium bubbles even under long-term annealing, which can inhibit the dissociation or migration of helium bubbles. As shown in Fig. 8(b) (c), helium bubbles tended to preferentially aggregate at oxide particles relative to grain boundaries, which was consistent with Liu’s research [39]. Molecular dynamics simulations can be employed to investigate the migration potential energy of helium bubbles towards grain boundaries and nano-oxide particles. It is speculated that the migration potential energy of helium bubbles towards nano oxide particles might be lower, but further research is needed to delve into the mechanisms governing the evolution of helium bubbles in the presence of nano-oxide particles. This will contribute to reducing helium embrittlement and lay a solid theoretical foundation in the field of helium irradiation resistance.
Helium bubbles on grain boundaries and dislocations
Figure 9 illustrates that within the annealing duration of 10 to 300 h, 96% of helium bubbles are distributed in proximity to dislocation structures, signifying a significant influence of these structures on the bubble growth process. In Fig. 9(a) and (d), helium bubbles are notably aggregated along dislocation lines and complex dislocation structures. This observation suggests that complex dislocation structures exhibit strong adsorption and constraining effects on the helium bubbles. The micrograph shows that the helium bubbles on the dislocations are larger than those within the grains. This indicates that dislocations act as strong sinks and rapid diffusion paths for helium, causing bubbles to diffuse into shallow layers [26]. The bubble size and relative frequency of helium bubbles aggregating at the dislocations were counted and are depicted in Fig. 10. There was no significant difference in the size and frequency of helium bubbles between the LPBF and rolled samples for the 10 h PIAed samples. In the 100 hours PIAed samples, however, an obvious helium bubble coarsening is occurred in the rolled sample with the bubble size ranging from 10 nm to 11.5 nm but from 8 nm to 10 nm in the LPBF sample. The proportion of large-size bubbles in the rolled sample was noticeably higher, with the maximum size even reaching 15 nm compared to the LPBF sample. With the annealing time extended to 300 h, the growth and evolution of helium bubbles tended towards stability in both the rolled and LPBF samples, with the bubble size and density remaining basically unchanged and the bubble size distribution remarkably similar, as shown in Fig. 7 and Fig. 10. The average bubble size is 10 to 12 nm for 300 h, compared to 10–11.5 nm for 100 h in rolled samples, and 8 to 10 nm for 100 h, compared to the 8.5–10.5nm for 300 h in LPBF samples. In contrast, most of the cellular subgrains were decomposed in the LPBF sample after 300 h of annealing, but many dislocations were still retained.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F009.jpg)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F010.jpg)
It is well known that the aggregation of helium bubbles at grain boundaries can cause intergranular cracking, which seriously affects the mechanical properties of materials. Therefore, it is essential to study the evolution behavior of helium bubbles at the grain boundaries. As shown in Fig. 11, helium bubbles are notably concentrated and distributed along grain boundaries with a larger size than those nearby the boundaries in both the rolled and LPBF samples. The bubble size increased with annealing time. This observation suggests that grain boundaries serve as effective sinks for point defects, facilitating the rapid nucleation and growth of helium bubbles at grain boundaries. The size distribution of the bubbles at the grain boundaries was statistically counted and is shown in Fig. 12. The LPBF samples exhibited restrained bubble coarsening with smaller helium bubble sizes than the rolled samples, indicating excellent resistance to helium irradiation. El-Atwani et al. [40] proposed that different orientations of grains can affect the size and density of helium bubbles. Helium bubbles are more likely to aggregate and grow along the [110] direction [41]. However, because multiple grains were not observed in this study, a detailed discussion on this aspect was not pursued.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F011.jpg)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F012.jpg)
Discussion
Dependence of helium bubble evolution on annealing time
After annealing at 700 °C for 10,100, and 300 h, the bubble sizes of the irradiated samples follow the order A1<T1<T2<A2<A3<A4<T3<T4, showing slight discrepancies compared to previous research findings [32]. To investigate the underlying reasons, we simulated the curve of the density of helium bubbles with the reciprocal of the annealing temperature, conforming to Arrhenius law. The apparent activation energy
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F013.jpg)
Vacancy mechanism:_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M001.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M002.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M003.png)
At low temperatures, the activation energy corresponding to the displacement mechanism is 0.43–0.56 eV [42, 43], and the vacancy migration energy is 1.0–1.3 eV [22, 44, 45]. At high temperatures, the dissociation energy corresponding to helium is approximately 3.0 eV [46]. In this study, helium atoms tended to diffuse more through the displacement mechanism.
The stability of helium bubbles is affected not only by the diffusion of helium atoms but also by the overall aggregation and coarsening of the bubbles [4, 47]. It is well known that migration and coalescence (MC) and Ostwald ripening (OR) are the two main coarsening mechanisms during the growth of helium bubbles, with different pressures within the bubble triggering different coarsening mechanisms. The Carnahan-Starling hard sphere equation of state provides a good approximation [48]:_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M004.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M005.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M006.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M007.png)
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-M008.png)
Based on the above analysis, it is speculated that the samples within 10 h of annealing have not yet reached the thermal equilibrium state. Therefore, helium atoms tend to diffuse more through the displacement mechanism, where the lattice position of He atoms is occupied by self-interstitial atoms (SIA) and transitions to the interstitial position. The migration and coalescence of the helium bubbles occured. As the higher sink strength in the LPBF sample reduces vacancy supersaturation, the high-density dislocations in the LPBF samples act as the primary source of He atoms during annealing [51]. The re-release of helium atoms results in more helium bubbles migrating and aggregating in the form of helium atom clusters, and smaller He clusters exhibit higher mobility [52], resulting in a slightly larger helium bubble size in the LPBF sample than in the rolled sample. The specific mechanism is illustrated in Fig. 14.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F014.jpg)
Effect of intrinsic structure on the evolution of helium bubbles in LPBF 304L SS
It is well known that the existence of various defect structures in material systems can affect the evolution of helium bubbles. During annealing for 10–100 hours, the helium bubbles aggregated at the oxide particle-matrix interfaces in the matrix (Fig. 8). This underscores their efficacy in restraining the growth of helium bubbles as sinks for point defects. Although this effect diminished after 300 h of annealing, it effectively inhibited the migration and coalescence of helium bubbles during their nucleation and rapid growth in the early stages. In contrast, helium bubbles exhibited strong aggregation and dense distribution at the cellular subgrain boundaries composed of dislocations throughout the matrix (Fig. 9), indicating the effective capture of helium bubbles by dislocations. The fundamental reason is that helium atoms tend to diffuse to dislocations with lower potential energies for nucleation and growth [12]. Regarding bubble growth during annealing, the dislocation lines serve as primary sources for vacancies, which have a strong affinity for helium atoms, making them more likely to aggregate and partially confined to the dislocation mesh [51]. The high-density dislocations in the LPBF samples were more effective in dispersing helium into smaller bubbles (Fig. 10), whereas in the rolled sample, the absence of high-density dislocations leaded to more pronounced coarsening of helium bubble sizes at dislocations. It was confirmed that high-density dislocations have a strong adsorption and confinement effect on helium bubbles and remain relatively stable even after 300 h of annealing.
The same results of helium bubble aggregation were also obtained at the grain boundaries (GB) (Fig. 11). The helium bubbles in the GBs of the LPBF sample were significantly smaller than those in the rolled sample. The bubbles at the grain boundaries in the rolled samples coarsened and exhibited a pronounced tendency to aggregate. This indicates that there are no strong defect sinks in the rolled sample to inhibit the growth of helium bubbles, and the nucleation of helium bubbles along the grain boundaries is likely to be assisted by enhancing the diffusion of helium along the grain boundaries, which occurs at lower activation energies [52, 53]. After 100 h of annealing, larger helium-vacancy complexes became movable and were captured by grain boundaries, resulting in the net growth of helium bubbles [31, 54].
In contrast, LPBF 304L stainless steel has an abundance of interfaces, such as the high dislocation density around the cellular subgrains and the nano-oxide-matrix interface (Fig. 15) serve as capture sites for point defects. During the helium atom diffusion stage, these interfaces significantly enhanced the recombination of vacancies and interstitials. The depletion of vacancies inhibits the binding of vacancies and helium atoms and prevents the formation of helium bubbles [55, 56]. Regarding the nucleation stage of helium bubbles, these interfaces provide numerous nucleation sites for helium bubbles, which effectively disperse the aggregation of helium bubbles at grain boundaries and keep helium bubbles below the critical size for the bubble-to-cavity transition. Thus, the occurrence of helium embrittlement is reduced [50]. For the helium bubble growth stage under annealing, the high density of dislocations in the LPBF sample impedes the migration and merging of helium bubbles, inhibiting the overall coarsening of helium bubbles (Fig. 6) [57, 58].
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F015.jpg)
It can be concluded that the high density of dislocations and nano-oxide particles in the LPBF sample can effectively mitigate radiation hardening and high-temperature He embrittlement, thereby extending the working time of structural materials in nuclear energy systems.
Swelling caused by helium bubbles
To compare the dependence of the swelling rate on annealing time, the swelling degree in the peak-damage area was calculated for the LPBF and rolled samples, as shown in Fig. 16 [59]. When the annealing time was increased to 10 h, the material swelling rate was very weak with the extension of annealing time, and the two states of the samples exhibited almost identical material swelling. The rapid expansion of material swelling occurred in the period from 10 h to 100 h, especially the sharply increased swelling rate for the rolled sample but moderately for the LPBF samples because of the high density of dislocations. At the 100 h annealing time, the swelling rates of the rolled and LPBF samples were 3.2% and 1.47%, respectively. In LPBF samples, the presence of low-density and small helium bubbles reduces the overall swelling value [19]. This indicates that high-density dislocations are effective sinks for restricting the coarsening of helium bubbles by limiting their migration and aggregation of helium bubbles.
_2026_02/1001-8042-2026-02-31/alternativeImage/1001-8042-2026-02-31-F016.jpg)
The capture effect of nano oxide particles on helium bubbles was relatively weak compared to dislocation walls in LPBF 304L stainless steel, representing only a small amount of helium bubbles captured by the nano-oxide particle interfaces, along with the very small number of nano-oxide particles through the LPBF 304L stainless steel (Fig. 16). Therefore, it can be concluded that the dislocation structure in LPBF plays a major role in inhibiting the migration and growth of helium bubbles, and the sink strengths of dislocations (2.4 × 1014 m-2) is approximately one order of magnitude higher than that of nano-oxide particles (2.1 × 1013 m-2) [20]. Moreover, the stability of the dislocation structure surpasses that of nanoscale oxide particles after prolonged high-temperature annealing. This indicates that the high-density dislocations in the LPBF samples exhibit superior resistance to radiation-induced swelling compared with nanoscale oxide particles.
Conclusion
In this study, helium ion irradiation experiments were conducted at room temperature and annealed at 700 °C for 10,100 and 300 hours respectively to investigate the growth behavior of helium bubbles in LPBF 304L compared with conventionally rolled counterpart. The main conclusions are as follows:
Nucleation behaviour of helium bubbles in LPBF: The depth of the helium bubble damage zone in LPBF samples is approximately 950 nm, the width is approximately 430 nm, and the density of helium bubbles in the peak helium concentration zone is 1.12 × 1024 m-3. The depth of the helium-induced damage zone in the rolled samples is about 980 nm, the width is about 470 nm, and the density of helium bubbles in the peak helium concentration zone is 3.86 × 1024 m-3. TEM revealed that the nanoprecipitates and high-density dislocations in LPBF can act as defect sinks to trap and annihilate point defects, and the LPBF samples have narrower irradiation damage regions and lower helium bubble densities. Therefore, LPBF samples have superior resistance to helium bubble nucleation.
Helium bubble growth behaviour and swelling behaviour of LPBF samples: the size of helium bubbles in rolled and LPBF samples increases and the density decreases with annealing time. After annealing for 10 hours, the helium bubble size in LPBF samples is slightly larger than in rolled samples, which is due to the fact that the irradiated samples are in a state of disequilibrium. The surface activation energy (Eact) was calculated using by the Arrhenius model, which determined that helium atoms tend to diffuse through the substitution mechanism, and helium bubbles grow under the migration and coalescence (MC) mechanism. Annealing for 10–100 h is the period of rapid growth of helium bubbles, and after annealing for 1000–300 h the bubbles enter a period of stable growth. Compared with the rolled samples, the LPBF samples have lower swelling coefficients after the post-irradiation annealing treatment, so it can be speculated that the LPBF samples have excellent resistance to helium bubble coarsening.
Microstructure of LPBF samples: during the annealing period of 10–100 h, the cellular subgrains and the oxide nanoparticles of the material remain stable and have a strong trapping effect on helium bubbles, and after annealing for 300 h, the cellular subgrains begin to decompose and the oxide nanoparticles no longer provide trapping for helium bubbles, which indicates that the oxide nanoparticles are not as stable as high-density dislocations, and at this time, the high-density dislocations become the main factor inhibiting helium bubble growth in LPBF samples. The LPBF samples still have excellent resistance to helium irradiation in a long-term service environment.
High mechanical strengths and ductility of stainless steel 304L fabricated using selective laser melting
. J. Mater. Sci. Technol. 35, 388 2019). https://doi.org/10.1016/J.JMST.2018.10.013Characterization of laser spatter and condensate generated during the selective laser melting of 304L stainless steel powder
. Addit. Manuf. 31,Influence of Ti, C and N concentration on the intergranular corrosion behaviour of AISI 316Ti and 321 stainless steels
. Acta Mater. 55, 2239 2007). https://doi.org/10.1016/J.ACTAMAT.2006.11.021Helium accumulation in metals during irradiation - Where do we stand?
J. Nucl. Mater. 323, 229 2003). https://doi.org/10.1016/j.jnucmat.2003.09.001Radiation-induced helium bubbles in metals
. Materials (Basel). 12, 1036 2019)The influence of microstructure on blistering and bubble formation by He ion irradiation in Al alloys
. J. Nucl. Mater. 467, 357 2015). https://doi.org/10.1016/j.jnucmat.2015.09.051Evaluation of Helium effects on swelling behavior of oxide dispersion strengthened ferritic steels under ion irradiation
. J. Nucl. Mater. 367–370, 423 2007). https://doi.org/10.1016/J.JNUCMAT.2007.03.016Helium-bubble formation and void swelling in nimonic PE16 alloy under dual-ion (He+, Ni+) irradiation
. Nucl. Instruments Methods Phys. Res. 209–210, 381 1983). https://doi.org/10.1016/0167-5087(83)90827-XHigh-temperature helium embrittlement of 316FR steel
. J. Nucl. Sci. Technol. 48, 130 2011). https://doi.org/10.3327/jnst.48.130Helium in fusion materials: High temperature embrittlement
. J. Nucl. Mater. 133–134, 100 1985). https://doi.org/10.1016/0022-3115(85)90118-7Methylphenylethynylpyridine (MPEP) Novartis
. Curr. Opin. Investig. Drugs. 1, 355 2000)Designing radiation resistance in materials for fusion energy
. Annu. Rev. Mater. Res. 44, 241 2014). https://doi.org/10.1146/annurev-matsci-070813-113627Microstructural development under irradiation in European ODS ferritic/martensitic steels
. J. Nucl. Mater. 351, 247 2006). https://doi.org/10.1016/J.JNUCMAT.2006.02.005The effect of Ar-ion irradiation on nanomechanical and structural properties of ODS RAF steels manufactured by using HIP technique
. Vacuum. 145, 144 2017). https://doi.org/10.1016/J.VACUUM.2017.08.039Effects of ion irradiation on microstructure of 316L stainless steel strengthened by disperse nano TiC through selective laser melting
. Mater. Charact. 180, 2021). https://doi.org/10.1016/j.matchar.2021.111420Effects of interfaces on the helium bubble formation and radiation hardening of an austenitic stainless steel achieved by additive manufacturing
. Appl. Surf. Sci. 467–468, 1134 2019). https://doi.org/10.1016/j.apsusc.2018.10.268Effect of LaB6 addition on mechanical properties and irradiation resistance of 316L stainless steels processed by selective laser melting
. Int. J. Adv. Nucl. React. Des. Technol. 3, 74 2021). https://doi.org/10.1016/j.jandt.2021.06.004Microstructure, tensile properties and mechanical anisotropy of selective laser melted 304L stainless steel
. J. Mater. Sci. Technol. 48, 63 2020). https://doi.org/10.1016/J.JMST.2020.01.011Effect of helium bubbles on irradiation hardening of additive manufacturing 316L stainless steel under high temperature He ions irradiation
. J. Nucl. Mater. 550, 2021). https://doi.org/10.1016/j.jnucmat.2021.152948Helium bubble nucleation in Laser Powder Bed Fusion processed 304L stainless steel
. J. Nucl. Mater. 542,Helium desorption behavior and growth mechanism of helium bubbles in FeCrNi film
. Nucl. Mater. Energy. 21, 2019). https://doi.org/10.1016/j.nme.2019.100710Temperature dependence of bubble structure in 316L stainless steel irradiated with 2.5 MeV He ions
. J. Nucl. Mater. 258–263, 1623 1998). https://doi.org/10.1016/S0022-3115(98)00332-8Bubble formation in helium-implanted nanostructured ferritic alloys at elevated temperatures
. Acta Mater. 217, 2021). https://doi.org/10.1016/j.actamat.2021.117165Evolution of helium bubbles in SLM 316L stainless steel irradiated with helium ions at different temperatures
. J. Nucl. Mater. 562, 2022). https://doi.org/10.1016/j.jnucmat.2022.153609Helium bubble evolution and hardening in 316L by post-implantation annealing
. J. Nucl. Mater. 500, 389 2018). https://doi.org/10.1016/j.jnucmat.2018.01.017Helium bubble formation in 800 MeV proton-irradiated 304L stainless steel and alloy 718 during post-irradiation annealing
. J. Nucl. Mater. 304, 1 2002). https://doi.org/10.1016/S0022-3115(02)00874-7Helium solubility and bubble formation in a nanostructured ferritic alloy
. J. Nucl. Mater. 445, 165 2014). https://doi.org/10.1016/j.jnucmat.2013.10.048In-situ TEM observation of microstructure evolution in Fe9Cr1·5W0·4Si alloy during He+ irradiation and post-implantation annealing
. J. Nucl. Mater. 555,Microstructure evolution during helium irradiation and post-irradiation annealing in a nanostructured reduced activation steel
. J. Nucl. Mater. 479, 323 2016). https://doi.org/10.1016/j.jnucmat.2016.07.030Helium bubbles in FeNiCr after post-implantation annealing
. J. Nucl. Mater. 212–215, 336 1994). https://doi.org/10.1016/0022-3115(94)90082-5Thermal stability of nanoscale helium bubbles in a 14YWT nanostructured ferritic alloy
. J. Nucl. Mater. 445, 84 2014). https://doi.org/10.1016/j.jnucmat.2013.10.024Helium bubble growth in He+ ions implanted 304L stainless steel processed by laser powder bed fusion during post-irradiation annealing at 600 °C
. Acta Metall. Sin. (English Lett. 35, 1509 2022). https://doi.org/10.1007/s40195-022-01391-wHelium bubble nucleation in laser powder bed fusion processed 304L stainless steel
. J. Nucl. Mater. 542,SRIM - The stopping and range of ions in matter (2010)
, Nucl. Instruments Methods Phys. Res. Sect. B Beam Interact. With Mater. Atoms. 268, 1818–1823 2010). https://doi.org/10.1016/j.nimb.2010.02.091Helium bubble growth in He+ ions implanted 304L stainless steel processed by laser powder bed fusion during post-irradiation annealing at 600 °C
. Acta Metall. Sin. (English Lett. 35, 1509 2022). https://doi.org/10.1007/s40195-022-01391-wAluminum parts fabricated by laser-foil-printing additive manufacturing: Processing, microstructure, and mechanical properties
, Materials (Basel). 13 2020). https://doi.org/10.3390/ma13020414Effect of Cold-Rolling Reduction on Recrystallization Microstructure, Texture and Corrosion Properties of the X2CrNi12 Ferritic Stainless Steel
, Materials (Basel). 15 2022). https://doi.org/10.3390/ma15196914Irradiation-tolerant nanostructured ferritic alloys: Transforming helium from a liability to an asset
. Jom. 62, 84 2010). https://doi.org/10.1007/s11837-010-0144-1Effects of grain boundaries and nano-precipitates on helium bubble behaviors in lanthanum-doped nanocrystalline steel
. Scr. Mater. 200,The role of grain size in He bubble formation: Implications for swelling resistance
. J. Nucl. Mater. 484, 236 2017). https://doi.org/10.1016/j.jnucmat.2016.12.003Crystal orientation dependence of surface modification in molybdenum mirror irradiated with helium ions
. J. Nucl. Mater. 455, 297 2014). https://doi.org/10.1016/j.jnucmat.2014.06.030Helium bubble formation in nickel during hot implantation
. J. Nucl. Mater. 212–215, 358 1994). https://doi.org/10.1016/0022-3115(94)90086-8TEM study of the nucleation of bubbles induced by He implantation in 316L industrial austenitic stainless steel
. J. Nucl. Mater. 466, 646 2015). https://doi.org/10.1016/j.jnucmat.2015.09.013Electrical resistivity recovery in Fe-Cr-Ni alloys after neutron irradiation at low temperature
. J. Nucl. Mater. 131, 53 1985). https://doi.org/10.1016/0022-3115(85)90424-6Modeling of helium bubble nucleation and growth in austenitic stainless steels using an Object Kinetic Monte Carlo method
. Nucl. Instrum. Meth. Phys. Res. Sect. B 352, 107 2015). https://doi.org/10.1016/j.nimb.2014.11.110The growth of helium bubbles in stainless steel at high temperatures
. Philos. Mag. A Phys. Condens. Matter. Struct. Defects Mech. Prop. 47, 781 1983). https://doi.org/10.1080/01418618308245265An analysis of the bubble formation behaviour under different experimental conditions
. J. Nucl. Mater. 186, 153 1992). https://doi.org/10.1016/0022-3115(92)90330-NAnalytical solutions for helium bubble and critical radius parameters using a hard sphere equation of state
. J. Nucl. Mater. 131, 118 1985). https://doi.org/10.1016/0022-3115(85)90450-7Helium bubbles in nickel annealed at T > 0.7 Tm
. 250, 103 1997). https://doi.org/10.1016/S0022-3115(97)00275-4The effect of internal pressure on the coarsening of inert gas bubbles in metals
. Scr. Metall. 23, 1773 1989). https://doi.org/10.1016/0036-9748(89)90359-1The effects of post-irradiation isochronous annealing on defects evolution and hardening in Hastelloy N alloy
. J. Nucl. Mater. 548, 2021). https://doi.org/10.1016/j.jnucmat.2021.152855Effects of temperature on helium bubble behaviour in Fe–9Cr alloy
. J. Nucl. Mater. 532, 2020). https://doi.org/10.1016/j.jnucmat.2020.152045Grain boundary diffusion in metals
. In Diffusion in Condensed Matter, ed. byHelium bubble nucleation at grain boundaries
. Philos. Mag. A Phys. Condens. Matter, Struct. Defects Mech. Prop. 48, 965 1983). https://doi.org/10.1080/01418618308244330Efficient annealing of radiation damage near grain boundaries via interstitial emission
. Science 327, 1631 2010). https://doi.org/10.1126/science.1183723Controlling radiation damage
. Science 327, 1587 2010). https://doi.org/10.1126/science.1188088Helium bubble distributions in a nanostructured ferritic alloy
. J. Nucl. Mater. 434, 210 2013). https://doi.org/10.1016/j.jnucmat.2012.11.049Radiation damage in helium ion irradiated nanocrystalline Fe
. J. Nucl. Mater. 425, 140 2012). https://doi.org/10.1016/j.jnucmat.2011.10.052The effect of injected interstitials on void formation in self-ion irradiated nickel containing concentrated solid solution alloys
. J. Nucl. Mater. 488, 328 2017). https://doi.org/10.1016/j.jnucmat.2017.02.026The authors declare that they have no competing interests.